Full synthesis process:

- Graphene oxide dispersion of 3-4 mg/ml of de-ionized water mixed uniformly with ethylenediamine at 20 μl/5ml and then sealed in a glass vial and heated for 6 -8 hours at 95 ° C (~205 ° F) for synthesis of functionalized graphene hydrogel (FGH).

- After cleaning in de-ionized water and freeze-drying, functionalized graphene aerogel (FGA) is produced.

- Last, the aerogel is exposed to MWI in an inert atmosphere for 1 min to give rise to the final ULGA.
Рекомендации по теме
Комментарии
Автор

This was satisfying on multiple levels. I could totally fall asleep to your voice lol.

reallyMika
Автор

This morning I had an asterisk above my head and searched YT for ~ Carbon Areogel. I love You Tube!

kenlee
Автор

More than Awesome, you promised this one ages ago lol.
But i forgive you ha ha can't wait for part 2 😎

mouldykev
Автор

Hi,
How did you put the container of essential oils in the oven? don't they melt?
where did you buy them?
Many thanks

CarmeloVita
Автор

Hi Kingswell Labs, may I know the molarity of the EDA? What is the properties of the reducing agent so that it able to reduce the GO to aerogel form? I used pyrrole but it ends up like a dust particles

FHSWorld
Автор

We are looking for a method to synthesize highly oxidized graphene oxide by electrochemical exfoliation.
How did you synthesize your graphene oxide?

OAI_FT
Автор

Hi, Kingswell Labs, I did enjoy your video it helped me a lot to understand the freeze-drying process, I have a question I don t want to synthesis an aerogel but a graphene oxide sponge. I use 10 mg/ml as a concentration and dispersed it in 200ml of water. after the ultrasonication process, I applied the hydrothermal method and freeze the solution before taking it to the freeze-dryer. but in the end, I did not get a sponge but the dust of particles. I try to understand what I have done wrong? Could you please assist? Thank you

shirleypriscillaonkani
Автор

I done it, but after removing the container from the oven, the separate particles were at the bottom of the container and were not compact and in a molded form. I cant find the problem that is very kind of you to help me to find the problem

amirmohammadhosseini
Автор

Sir ant alternative to EDA? Can I use DEA

ETMS.
Автор

Hi! do you mind to share the reference of the experimental procedure?

aristyosoecipto
Автор

Does the graphene oxide dispersion have to be 3-4 mg/ml? is it like the best concentration to use or can you use another concentration? Thank you!

creamcookies
Автор

Spin a variable electromagnetic cylinder in a beaker of graphite oxide solution, make sure the liquid is spinning within the container as a result of the em cylinder motion. Add in your reducing solvent dropwise and Increase the magnetic field strength slowly, watch your graphene aerogel crystal puk grow. You're welcome ftf

crb
Автор

Could you just use graphene instead of GO? I'm just not a fan of the modified hummers method to make GO

dedlunch
Автор

How do you remove the gel from the water without breaking it?

gianniskarnis
join shbcf.ru